Page 57 of 561
56
235
265
315
355
390
420
NV A NV B NV D NV E
NV A27S NV D27S NV E27S
NV A32 NV D32 NV E36
NV A36 NV D36 NV E36
NV A40 NV D40 NV E40
NV A420 NV D420 NV E420
Grade
Yield stress RcH minimum (MPa)
530 to 680
510 to 660
490 to 630
440 to 570
400 to 530
400 to 520
Tensile strength Rm (MPa)
18
20
21
22
22
22
Elognation A5 minimum (%)
Mechanical properties typical values
0 -20 -40
0 -20 -40
0 -20 -40
0 -20 -40
0 -20 -40
+20 0 -20 -40
Temperature (°C)
42
39
34
31
27
– 27 27 27
Impact energy L (J) t # 50 (mm)
E390CC E390DD E390E
Fe 510C Fe 510D E355E
– – –
Fe 430C Fe 430D –
Fe 360B Fe 360C Fe 360D –
ISO 630-80 4950/2/3 1981
S420N/M S420N/M S420NL/ML
S355N/M S355N/M S355NL/ML
– – –
S275H0G3 S275N/M S275NL/ML
S235JRG2 S235J0 S235J2G3 S275NL/ML
EN 10025-93 EN 10113-93
EN
AH40 DH40 EH40
AH36 DH36 EH36
AH32 DH32 EH32
– – –
A B D E
A 131
ASTM
(SM58) – –
SM53B (SM50C) –
SM50B (SM50C) –
– – –
SM41B SM41B (SM41C) –
G 3106
JIS
SOLUTIONS
2.04