Page 438 of 561

WIRE WELDING

Edge preparation

Aluminium, Position welding, Argon Shielding gas Material thickness mm

Type of Welding joint position *

Gas consumption l/min.

Wire diameter mm

Welding parameters Amp

Volt

Welding speed cm/min

Number of layers

60° 6.5 (1/4”)

V

20

1.2 or 1.6

180

23

50

2

60° 6.5 (1/4”)

OH

20

1.2 or 1.6

200

23-24

55

2

60° 9.5 (3/8”)

V

20

1.2 or 1.6

210

23

45

3

60° 9.5 (3/8”)

OH

23

1.6

220

23-24

50

3

60° 12.7 (1/2”)

V

23

1.6

215

22-23

30

3

60° 12.7 (1/2”)

OH

25

1.6

225

23-24

40

4

75° 19 (3/4”)

V

25

1.6

225

23-24

25

4

75° 19 (3/4”)

OH

25

1.6

240

24

35

6

V: Vertical, OH: Over head *4 mm (1/16”)

4 mm (1/16”)

Copper alloys, Horizontal, Argon Shielding gas Material Type of thickness joint mm

Gas consumption l/min.

Wire Welding parameters diameter Wire speed Amp Volt mm cm/min

3 (1/8”)

15-20

1.6

310

27

500

6.5 (1/4”)

15-20

2.4

460

26

345

90° 9.5 (3/8”)

5 mm

15-20

2.4

500

27

380

90° 12.7 (1/2”)

5 mm

15-20

2.4

540

27

420

4.03

NB: When welding Cunifer backing gas must be used 437